Which plastic will hold your cleaner without failing?
Updated
On this page10
For most water-based cleaners, high-density polyethylene (HDPE) is the safe first choice: the charts read for this page rate it well against dilute acids such as vinegar and citric acid, against alkalis such as washing soda and sodium hydroxide, and against ammonia and alcohols. Polypropylene (PP) behaves much the same and is what most caps and sprayers are made of. PET holds acids and alcohols but is rated poorly against alkalis. Bleach, peroxide and citrus oils are where the charts start to disagree or drop their ratings, and fluorinated HDPE exists for solvents. Every chart is a guide for pure chemicals, so the real answer comes from testing your product in your bottle.
The charts behind this page
No chart read for this page tests a finished cleaning product. Each one soaks plastic samples in single chemicals at stated concentrations and temperatures, then rates the damage. Their keys differ, so the table below keeps each source's own rating.
| Source | Plastics | Conditions | Rating key |
|---|---|---|---|
| Thermo Fisher (Nalgene) chemical resistance chart, 2022 [1] | LDPE, HDPE, PP, fluorinated PE (FLPE) and others | 20°C and 50°C; mostly pure chemicals | E no damage after 30 days; G little or no damage after 30 days; F some effect after 7 days; N immediate damage may occur |
| Th. Geyer, Chemical Resistance of LDPE, HDPE & PP, undated [2] | LDPE, HDPE, PP | 20°C and 50°C | ++ very good; + good; - poor, not recommended; -- no resistance |
| LyondellBasell, Pro-fax and Moplen Chemical Resistance, 08/2015 [3] | PP | ASTM D543, unstressed specimens, 1 month immersion, 20°C, 60°C, 100°C | A negligible effect; B limited absorption or attack; C extensive absorption or rapid permeation; D extensive attack |
| Corning, Chemical Resistance Comparison of PET and PETG, August 2017 [4] | PET, PETG | By chemical family, not single chemicals | 1 no damage after 30 days; 2 little to no damage after 30 days; 3 some effect after 7 days (crazing, cracking, loss of strength, discoloration); 4 not recommended for continuous use |
| Greiner Bio-One, Chemical Resistance of Various Materials, file dated October 29, 2021 [5] | PP, HDPE, LDPE, PS, PC; PET membrane at room temperature | 20°C and 50°C | 1 resistant; 2 limited; 3 moderate; 4 no resistance |
Th. Geyer's own caveat applies to all of them: "The mentioned resistance levels are only guide values" [2]. Thermo Fisher calls its chart "a general guide only" and says "you should test under your own conditions" [1]. Corning says testing "should be conducted for each specific usage condition" [4].
Ratings by what your product contains
Ratings are shown as 20°C / 50°C, except LyondellBasell's, which are 20°C / 60°C. Where a chart does not list a chemical, the cell says so.
| What the product contains | HDPE | LDPE | PP | PET |
|---|---|---|---|---|
| Vinegar and other dilute acids (acetic acid 10%, citric acid 10%) | Greiner 1/1 both [5]; Geyer acetic 50% ++/++, citric 10% ++/++ [2] | Greiner 1/1 [5]; Geyer ++/++ [2] | LyondellBasell acetic 10% A/A, citric 10% A/A [3] | Corning dilute acids 1 [4]; Greiner PET acetic 10% 1 [5] |
| Strong mineral acids (hydrochloric 20%, phosphoric 85%) | Geyer ++/++ both [2]; Greiner 1/1 [5] | Geyer ++/++ [2] | LyondellBasell hydrochloric 20% A, phosphoric 95% A/A [3] | Corning strong or concentrated acids 3 [4] |
| Concentrated sulfuric acid | Geyer 95%: -/-- [2]; Greiner conc. 4/4 [5] | Geyer -/-- [2] | LyondellBasell 98%: C at 20°C [3] | Not rated for this strength |
| Alkalis (sodium hydroxide, potassium hydroxide, washing soda) | Geyer NaOH 50% ++/++, KOH 50% ++/++, sodium carbonate ++/++ [2]; Nalgene sodium carbonate E/G [1] | Geyer ++/++ [2]; Nalgene sodium carbonate E/E [1] | LyondellBasell NaOH 10% and 50% A/A [3] | Corning inorganic bases 3 to 4 [4]; Greiner PET NaOH 4 [5] |
| Ammonia (25%) | Geyer ++/++ [2]; Greiner 1/1 [5]; Nalgene E/E [1] | Geyer ++/++ [2]; Nalgene E/E [1] | Nalgene E/E [1]; LyondellBasell ammonium hydroxide 10% A/A [3] | Greiner PET 5% ammonium hydroxide 1 [5]; Corning inorganic bases 3 to 4 [4] |
| Sodium hypochlorite (chlorine bleach) | Geyer 15%: ++/++, but "bleach solution, 12.5% chlorine": -/-- [2]; Greiner 2/3 [5] | Geyer 15%: ++/++ [2]; Greiner 2/3 [5] | LyondellBasell 20%: A/B [3]; Greiner 2/3 [5] | Corning dilute oxidizers 3 [4] |
| Hydrogen peroxide (3% to 10%) | Greiner 3%: 1/1 [5]; Geyer 10%: +/+ [2] | Greiner 3%: 1/1 [5]; Geyer 10%: +/+ [2] | LyondellBasell 3%: A [3] | Corning dilute oxidizers 3 [4] |
| Ethanol and isopropyl alcohol | Nalgene E/E both [1]; Geyer ++/++ [2] | Nalgene ethanol E/G, isopropyl E/E [1] | Nalgene E/E [1]; LyondellBasell 96% ethanol and 100% isopropanol A [3] | Corning aliphatic alcohols 1 [4] |
| Ethylene glycol | Nalgene E/G [1] | Nalgene E/E [1] | Nalgene E/E [1]; LyondellBasell A/A [3] | Greiner PET 1 [5] |
| Orange oil (citrus oil, d-limonene) | Nalgene G/F [1] | Nalgene G/N [1] | Nalgene G/F [1] | Not listed by name; Corning rates PET 3 for hydrocarbons as a family [4] |
| Turpentine | Geyer +/+ [2] | Geyer -/-- [2] | Geyer -/-- [2]; LyondellBasell C at 20°C [3] | Not listed by name |
| Mineral oil | Nalgene E/E [1] | Nalgene G/N [1] | Nalgene G/F [1]; LyondellBasell A at 20°C, B at 60°C [3] | Corning oils and greases 2 [4] |
| Detergents | Not rated in these charts; see stress cracking below | Not rated | LyondellBasell 2% detergents A/A/A [3] | Corning detergents and surfactants 2 [4] |
Reading the table for your product
Water-based cleaners with vinegar, citric acid, washing soda, borax or dish soap. Every chart that lists these chemicals rates HDPE, LDPE and PP well at the concentrations shown. The open question for HDPE and LDPE is stress cracking from the surfactant, covered below.
Anything alkaline in PET. Corning rates PET 3 to 4 against inorganic bases, and the Greiner PET table rates sodium hydroxide 4 [4][5]. Keep washing soda, sodium hydroxide and other high-pH products out of PET unless your own testing shows otherwise. PET does well with acids and alcohols in the same charts, so a vinegar glass cleaner is a reasonable candidate.
Bleach. The sources do not agree. Th. Geyer rates 15 percent sodium hypochlorite "very good" in HDPE and also rates a "bleach solution, 12.5% chlorine" poor [2]; Greiner rates hypochlorite only "limited" in HDPE, LDPE and PP [5]; LyondellBasell rates 20 percent hypochlorite as negligible effect in PP at 20°C [3]. LyondellBasell also explains a failure in PP that looks like stress cracking but is "caused by the strong oxidizing effect of the bleach" [6]. Treat bleach products as needing a full test in the real bottle, closure and liner, and expect gas pressure as well, which the venting page covers.
Peroxide. Dilute peroxide rates well in PE and PP in the charts that list it, and Corning puts PET at 3 against dilute oxidizers [3][4][5]. Thermo Fisher's advice for laboratory storage is blunter: "Do not store strong oxidizing agents in plastic labware except that made of Teflon FEP or PFA" [1]. A 3 percent product is not a strong oxidizer in the sense of a concentrated one, but test it, and plan for oxygen pressure.
Citrus oil and d-limonene. Only the Thermo Fisher chart lists orange oil, and it drops HDPE and PP to F (some effect after 7 days) and LDPE to N (immediate damage may occur) at 50°C [1]. At 20°C all three are G. For a degreaser with a meaningful share of limonene, that points to HDPE or fluorinated HDPE at minimum, and away from LDPE squeeze bottles, with a heat test before you commit.
Turpentine and other plant terpene solvents. Th. Geyer rates HDPE good and LDPE and PP poor to none [2], and LyondellBasell rates PP C, extensive absorption [3].
Environmental stress cracking
A bottle can pass a chemical soak and still split at the base or shoulder months later. That is environmental stress cracking (ESC): "the failure of a plastic material in the presence of certain types of chemicals" [1]. It needs three things at once: tensile stress in the plastic, a stress cracking agent, and a plastic susceptible to it. Common agents are "detergents, surface active chemicals, lubricants, and oils," and "Relatively small concentrations of stress cracking agent may be sufficient to cause cracking" [1]. That puts almost every cleaner, which is built on surfactants, in the at-risk group for polyethylene.
LyondellBasell's notes on polyethylene add the factors you can act on [7]:
- ESC failures "are accelerated by high temperatures and additional external stresses." A hot warehouse and a tall stack of cases make it worse.
- Lower density, higher molecular weight (lower melt index) and a narrower molecular weight distribution all increase stress crack resistance. Bottles for detergents, solvents or acids should be made from a resin with high stress crack resistance.
- The standard tests are ASTM D1693, a bent strip immersed in a surfactant solution at 50°C, and ASTM D2561, a test on filled bottles reported as the hours until half of them fail. LyondellBasell warns that "these methods are very sensitive to testing error; the data must be used with caution."
What this means for you: ask your bottle supplier which resin grade the bottle is blown from and whether it was chosen for stress crack resistance, and put your own filled bottles under heat and load in your test.
Fluorinated HDPE
Fluorinated HDPE bottles have had their surface treated with fluorine gas, which creates a fluorinated layer meant to cut permeation of hydrocarbon solvents and of polar liquids such as alcohols [8]. Ask the bottle supplier for its own permeation data on the treated bottle with a solvent close to yours.
In the Thermo Fisher chart, fluorinated PE rates E/G against orange oil where plain HDPE rates G/F [1]. The same chart rates it lower than HDPE against sodium carbonate (G/F against E/G) and ammonia (F/F against E/E) [1]. Choose it for solvent and citrus products, and keep plain HDPE for alkaline water-based cleaners.
Glass
None of the charts read for this page rates glass, so this page gives no ratings for it. Glass brings its own problems for a product you sell: breakage, weight, and the cushioning carriers expect around it, which the case packing page covers. For a homemade spray kept at home, the bottles and labels page explains when glass is the better choice.
Testing your product in the real bottle
The charts narrow the choice. Only a test with your formula, your bottle, your closure or sprayer and your liner tells you it works. If you ship a regulated hazardous material, 49 CFR 173.24(e) makes the shipper responsible for packaging that is compatible with its contents, naming corrosivity, permeability, softening, premature aging and embrittlement, and the permeation test it applies to plastic packagings of liquids runs at 18°C for 180 days, 50°C for 28 days or 60°C for 14 days [9]. Those times and temperatures make a sensible frame for a small maker's test even when the product is not regulated.
- Fill at least six bottles per condition with a released batch, closed with the closure or sprayer you will sell, filled to your normal height.
- Weigh each filled bottle on a scale that reads to 0.1 g and record it.
- Store one set at room temperature and one set warm, for example at 50°C for 28 days, following the 49 CFR frame. Keep a set upside down so the product sits against the liner or sprayer seals.
- Weigh and inspect weekly. Look at the base, the shoulder, the neck threads and the closure liner.
- At the end, check the product for pH, color, odor and clarity against your retained sample, and work the sprayer to see that it still primes and seals.
- Record everything with the bottle supplier's part number and resin, so a change of supplier triggers a new test.
The same filled bottles can serve your stability study; the shelf life for products you sell page covers what else to measure.
Signs that the product is attacking the bottle
| What you see | What it usually means | What to do |
|---|---|---|
| Steady weight loss with no leak | Permeation: a volatile ingredient (water, alcohol, solvent, fragrance) is passing through the wall | Compare against a water-filled control bottle; consider fluorinated HDPE for solvents [8] or a thicker wall |
| Sides sucked in (paneling) | Pressure inside has dropped below the room: permeation outward, or an ingredient reacting with the air in the headspace [10] | See the venting page; a vented liner equalizes pressure |
| Bottle bulging or domed base | Gas building inside; hypochlorite bleach is named as a gas-generating product that causes "bottle bulging and stress cracking" [10] | Vented closure and a check of the formula |
| Plastic soft, tacky or swollen | Absorption of the product into the plastic (LyondellBasell's C rating) [3] | Change resin; this is a material mismatch |
| Fine cracks, crazing or cloudiness | Chemical attack or the start of stress cracking (Corning's rating 3 describes crazing, cracking, loss of strength or discoloration) [4] | Stop using that bottle for this product and test a higher stress crack resistance resin |
| Splits at the base or shoulder after weeks | Environmental stress cracking, worse with heat and stacking load [1][7] | Ask the supplier for a higher stress crack resistance grade; reduce stack height and heat |
| Product changed color or smell | Extraction from the plastic, or an unrelated formula problem | Compare with product stored in glass; see the color change page |
From the bottle to the sprayer and cap
The bottle is half of the package. Sprayer seals, springs and cap liners meet the same product, often under more mechanical stress, and fail in their own ways. The triggers and sprayers page covers those parts, and the venting page covers products that make or consume gas.
Top picks
Top containers for cleaning
32 oz · 28-400 · HDPE · White · 9.7 in
32 oz · 28-400 · HDPE · Natural
32 oz · 28-400 · HDPE · White · 9.6 in
16 oz · 28-400 · HDPE
16 oz · 28-410 · HDPE
32 oz · 38-400 · HDPE
32 oz · 28-410 · HDPE
16 oz · 24-410 · HDPE
References
- Thermo Fisher Scientific, Nalgene chemical resistance chart for labware (COL25838 0122), 2022. https://qa1-assets.thermofisher.cn/TFS-Assets/LED/Specification-Sheets/D20480.pdf
- Th. Geyer GmbH & Co. KG, *Chemical Resistance of LDPE, HDPE & PP*, undated, read October 2026. https://www.thgeyer.com/fileadmin/media/labor/en/pdfs/downloads/produktinfos-kompatibilitaetslisten/th-geyer-chemical-resistance-of-ldpe-hdpe-pp.pdf
- LyondellBasell, *Pro-fax and Moplen Chemical Resistance* (ASTM), 08/2015. https://lyondellbasell.com/4a955f/globalassets/documents/polymers-technical-literature/Profax_and_Moplen_Chemical_Resistance_Guide_ASTM
- Corning Life Sciences, Application Note CLS-AN-461, *Chemical Resistance Comparison of PET and PETG*, August 2017. https://www.corning.com/catalog/cls/documents/application-notes/Application_Note_CLS-AN-461_Chemical_Resistance_Comparison_PETandPETG.pdf
- Greiner Bio-One, *Chemical Resistance of Various Materials* (technical appendix), file dated October 29, 2021. https://www.gbo.com/fileadmin/media/GBO-International/01_Downloads_BioScience/SALES_Product_Catalogues/Chemische_Bestaendigkeit_EN_20211029.pdf
- LyondellBasell, tech.topic, *Chemical Resistance of Polypropylene* (7972D/0715), undated, read October 2026. https://www.lyondellbasell.com/globalassets/documents/polymers-technical-literature/tech-topic-chemical-resistance-of-polypropylene.pdf
- LyondellBasell, tech.topic, *Environmental Stress Crack Resistance* (6892E/0715), undated, read October 2026. https://www.lyondellbasell.com/globalassets/documents/polymers-technical-literature/tech-topic-environmental-stress-crack-resistance.pdf?id=13944
- U.S. Patent and Trademark Office, U.S. Patent 5,244,615, *Process for the production of permeation resistant containers*, read October 2026. https://image-ppubs.uspto.gov/dirsearch-public/print/downloadPdf/5244615
- Legal Information Institute, 49 CFR 173.24, General requirements for packagings and packages, read October 2026. https://www.law.cornell.edu/cfr/text/49/173.24
- The Clorox Company, U.S. Patent 6,626,311 B2, *Selectively venting and load-sealing closure*, granted September 30, 2003. https://patents.google.com/patent/US6626311